Cyandiation of the Fine Fraction - 325

 

Conditions

  • Weight of the sample    = 0.300 Kg.
  • Solid-liquid relation      = 1:3
  • Percentage of cyanide   = 0.13%
  • pH                                 = 10.5
  • Time of contact             = 24, 48 and 72 hours.

Concentration of Thick Fraction + 325

Fraction Flotation

- Grinding

  • Weight of the sample      1.00 Kg.
  • % of solids                       50%
  • Time                                5 minutes
  • pH                                    7.4

- Rougher Flotation

         Reactives                                         K/TM

  • Aeropromotor 404                        0.030
  • Aerofloat 242                                0.020
  • Aeroxanate 350                             0.050
  • Pine oil                                          0.020
  • Conditioning                                       8 minutes
  • Foaming                                              5 minutes

- Scavenger Flotation

         Reactives                                         K/TM

  • Aeropromotor 404                        0.020
  • Aerofloat 242                                0.010
  • Aeroxanate 350                             0.020
  • Pine oil                                          0.010
  • Conditioning                                       5 minutes
  • Foaming                                              4 minutes
  • - Cleaning
  • Without reactives
  • Conditioning                                       5 minutes
  • Foaming                                              4 minutes

 